Blacksmithing | Can a File Make a Good Knife?

How to Make a Knife From a File?


I have a bunch of old and fairly new files of all sizes. I would like some information on the proper procedure in turning them into a decent blades.

Hi
Files can make decent knives but you have to do a fair bit of preparation first. To truly make a good knife I would suggest grinding all the teeth off so you are down to bare metal. If you forge the blade and the tang leaving the teeth on. All the valleys at the bottom of the teeth make small creases in the surface of the blade.

When you heat treat the blade these creases can form cracks or potential cracks, and are always a point of weakness.

In general file steel can be an unknown tool steel and I have heard there is considerable variation in quality. I would try quenching in oil for most. I would actually recommend buy new steel. O1 drill rod is easy to get and makes a good knife and most importantly you know what you are getting. Buy 3/4 or 1 inch round and just forge it flat then make your knife from that.

It might seem a little expensive to spend $30 or $40 on a piece of steel 3 feet long. If your knife breaks in the final heat treating after spending 10 to 20 hours on it the $10 spent on the piece of O1 used for the other knife seems pretty cheap.

If you are stuck for finding O1 and tool steel in your area try clicking through to Onlinemetals.com They carry a full range or sizes.

I have had a number of knife making requests lately so I am planning on doing a newsletter series on it in the near future.

I hope this helps.
David Robertson
Artist Blacksmith

Tuesday, May 11, 2010

How to Deaden The Noise of an Anvil ?

How Do I Decrease the Ring of My Anvil?



Hi
There are a couple of tricks to deaden the noise of an anvil a bit.

I do use a chain but the secret here is that it is a fairly heavy chain and you wrap it around the anvils waist. Then it must be bolted down very tightly to the stump or stand that supports the anvil. This does help deaden the ring significantly. The idea is to tightly clamp the anvil to its base with the chain.


You can also add a good sized magnet under the horn or the tail of the anvil. This will collect scale but it helps remove some of the ring as well.

Another option that I don't like as well as the others is to take a short length of chain and make a loop out of it and hang a weight off it. Then place the loop over the horn or the tail of the anvil. It too will help deaden it down the noise a bit, but as soon as you need that spot on the anvil it is in the way and has to be moved.

Hope this helps.

David Robertson
Artist Blacksmith

Monday, May 10, 2010

How to Avoid Distortion Heat Treating Damascus

How Do I prevent Scale Build up When Heat Treating a Knife?



Well making my third Damascus knife 13 layers ,when i get it polished and to the point of tempering when i put it in the gas kiln red hot to loose magnetic it warped every which way .made out of all the same coil spring steel and hammer welded plus all sorts of slag all over it now so while it was red hot gently hammered it straight again and annealed . so how can i get it polished perfect and temper with out slag and distortion next time now after i sand and polish it again ? whats to keep it from happening the next time I go to temper it ???


Hi
This is a little tricky to answer as I have not seen all the steps that you have gone through.
Slow cooling (annealing) in vermiculite or wood ash to relieve the stresses is very important. This should remove much of the tension between the two different types of steel. This should help reduce the warpage when you heat for quenching.

If you are heating the blade in a gas forge hold it so that the back is up and it heats evenly from both sides this should help with the distortion as well. It should only be heated just past the magnetic point. It doesn't have to get super hot. Then pull the blade out and test with a magnet until it just pulls then quench the whole thing in the appropriated quench medium. Water or oil. Then temper evenly 425 degrees in a toaster oven. Then a quick sanding and hold the edge in a water bath (about 1/4 inch deep) and paint the temper colors on the back with a torch. Blue on the back straw on the edge.

Then sand to final finish always keeping the edge and the blade cold by dipping in water.

In short I rough grind and sand to about 80 grit before I heat treat. The final sanding is done after the blade is hardened. When I harden there will be some scale formation but it is really very little as it is only up to color for about a minute and not very hot. Just enough to lose the magnetism.

I know some people use a nickel foil to wrap around their blades so that it doesn't oxidize very much. I have not used this technique but understand it works well. You would have to source a knifemaking supplier for the nickel foil.

Hope this helps.

David Robertson
Artist Blacksmith

Tuesday, April 27, 2010

Blacksmith Coal Forge Hood and Chimney

What do you need to take the coal smoke away from the forge when you build a coal forge?



I fire mostly propane so fume exhaust is a little bit less of a problem.
Coal forges definitely require a chimney to exhaust the smoke. There is a great deal of smoke
created when you burn coal.

Essentially you have two options
The first is the easiest and that is to make a large funnel shaped sheet metal hood to catch the smoke. It should enter into a 10 inch pipe (much smaller does not draft well for a coal forge. 8 inch diameter you take your chances on) This pipe should extend through your roof and ideally be 2 feet above the ridge line of the building. If you are in an area that requires building codes to be inforced you may have to use insulated stove pipe.

Coal smoke is actually much cooler than wood smoke and in reality does not need the insulated pipe but the building inspectors have no reference for this.
This hood works moderately well. You can start the draft by crumpling a couple of sheets of newspaper and lighting them on fire when you start the coal. Once the draft is started it is pretty easily maintained with the heat of the coal fire.
The second option is more complicated to construct. But works well. It is a Side draft chimney.
For plans google "side draft forge" or "side draft chimney for forge" you should be able to find something. It is basically a box that has a low opening in the side and a shelf inside the box that catches the smoke. The chimney draft sucks the smoke to the side and out of the way.

Good ones work very well. Again you may have to discuss chimney designs and materials with your building inspector.

Coal produces alot of smoke on start up, then simmers down as it converts to coke. Hardly any smoke with a coke fire. Charcoal works well too with very little smoke although you need some chimney to carry the fumes away from your work area.

I hope this helps. Good luck building your forge. Coal forge is the most versatile but it is a bit of a trick to get on to. It is also the easiest to build.

Take Care
David Robertson Artist Blacksmith

Thursday, March 18, 2010

Blacksmithing : Anvil Height

What is The Best Height For My Anvil?



Hi David
Thanks for all your emails they are really inspirational, I have just got my old gas forge, anvil and leg vice back off my uncle who never used it a bit rusty but no worse for wear, my question is this I have read somewhere that the correct height for a anvil is if you stand up straight with your arm down by your side and make a fist the height from the floor to your knuckles would be the ideal height to the top face of the anvil is the correct, my anvil and steel stand is about that height but it just feels a bit low for me? the other thing is if I use a stump of wood as a anvil stand what is the best wood to use?

Many of the old books on blacksmithing use this standard for anvil height. I too have always found this a bit low for several reasons. If your arm is close to full extension, the repeated impact can damage your tendon in the elbow if not the joint as well.

I have my primary anvil set at wrist height as I stand beside it. This creates more flex in the arm acting as more of a shock absorber. I do lose a little power having this flex but I prefer to err on the side of self preservation.


The other issue is that the lower the anvil is placed the more you will find yourself bending over. This creates strain on your back. Some thing to be avoided in later years. This is especially true of light work where you tend to get closer to see what is going on. Heavier work should be done in a more vertical position.

Mounting the anvil.

Mounting on a stump is good. I am not sure that the type of wood makes as much of a difference as the weight. I have seen some steel anvil stands (3 leg) that were quite heavy and worked well. The important part of this is that the anvil needs to be bolted securely down to the stump. This effectively adds the weight of the stump or stand to the anvil. In some cases this could add an extra 100 lbs. If the anvil just rests on top it, it looses efficiency as it bounces around.

This will help in the stability and the performance of the anvil.


A box filled with concrete with bolts for tieing down could be effective. I don't like the sand boxes as the anvil floats too much on top and you have to keep leveling it.

A lot comes back to personal preferences, but this is what I have prefered in the past.
Hope this helps.

David
www.artistblacksmith.com

Monday, February 15, 2010

What Finish to put on My Vine Arbour?

What Finish Is Suitable for my Blacksmith Forged Vine Arbour?



I want to protect the steel from rusting but be able to see the texture of the vines I made underneath. What are your suggestions?

Hi
Finishes in blacksmithing are always a question. Something like this I would use an automotive paint with an epoxy primer coat. The hard acrylic top coat protects for several years (about 7 in a low salt environment). The metal must be clean sandblasted and a good deal of care has to be used in applying the paint.

The nice thing with this paint (see an automotive supply store for it) is that it comes in almost any color and it is quite durable.

Your next option is to have all the pieces hot dipped galvanized. Then paint over top. The problem with this is that the galvanizing fills in the texture that you have worked so hard to create. It will provide a good long lifespan before rust develops, but is better suited for large scale curves and shaping.
Not so much for texturing on bars.

Another product that smiths in the states have had good luck with is called Permalaq (just google it for more info) It is a clear laquer that is sparyed on leaving the natural steel tone and is quite durable. Talk to the manufacturer for details of use, as I have not used it yet.

There is a longer article on the main website about finishes that may be worth reading.
Click on Blacksmithing Articles to see a full list of articles on the site.

Hope this helps
David
Artist Blacksmith


Monday, February 1, 2010

Blacksmith Spring Fuller Questions

Spring Fuller Suggestions for Blacksmithing



Mr. Robertson,
I would like to fabricate a hardy spring fuller.

I have several leafsprings from an old truck that I can use for the spring portion. I had figured I would shape each end of the spring in a swage to fit a 3/4" diameter bar and then weld 3 or so inches of the bar in place at each end of the spring. I would then bend the spring so that the round bars come together and finish by welding a piece of square stockon the outside of the spring to fit my hardy hole.

I have two questions. First, is it acceptable to use mild steel for the 3/4"fullers provided I keep them cool during use?

Second, what sort of heat treatment do I need to do on the leaf springs where they were heated and bent?

Hi
A couple of things.
The leaf spring may be too heavy to get a good spring action. I usually use a coil spring that I straighten out. Then flatten out the midle section to a thickness of about 1/4 inch. This gives enough of a spring.When welding either the hardy stem or the "jaws" onto the spring steel, preheat the spring steel to at least 500 degrees F. I will usually take them up untill they just show a bit of color perhaps 1200 F. This seems to work pretty well for me.

The mild steel will work fine for the jaws, at least for quite a while. Expect some wear though.

Once the spring is forged flat and bent to shape, Take an even dull orange heat on it and just let it air cool and it seems to work fine. The steel itself is springy will work just with normalizing. If you want to heat treat, temper to about 500 degrees F but this is not really required on this tool.

I have also made spring fullers using mild steel flat bar as the spring. 3/16 by 1.5 inches or 1/4 by 1 inch Both of these have worked as well.

Hope this helps.